40366 Chap.5 Tensile Testing and Charpy Impact
Tensile Testing and Charpy Impact
Two tests, two kinds of loading
This lab compares how materials respond to a slow pull and to a sudden blow. In the tensile part, Perspex, steel and aluminium in two heat-treatment conditions are pulled to failure on machines that record force and crosshead displacement, with no extensometer on the specimen.
In the impact part, notched steel specimens are broken by a pendulum at chosen temperatures, and the energy each absorbs is read from the machine.
Before testing, microstructure images and fractured samples are examined so that predictions can be made and then revisited.
From readings to properties
Engineering stress is force divided by the original cross-sectional area, and the tensile strength is its maximum, which can come before fracture as the specimen necks.
Elongation after fracture is measured from gauge marks once the broken halves are fitted together, never from the crosshead travel. Young's modulus and a 0.2% proof stress need a genuine strain measurement and are treated as an extension.
Reading impact results
Absorbed energy is plotted against temperature for each steel, with individual points kept visible.
The result indicates impact toughness under the test conditions only; it is not fracture toughness or a safe design load, and an exact transition temperature needs more data and an agreed criterion.
What this chapter covers
- 01
Force and crosshead displacement records
- 02
Engineering stress and original area
- 03
Tensile strength as the peak stress
- 04
Elongation after fracture from gauge marks
- 05
Test standards and loading speed
- 06
Young's modulus and the 0.2% offset
- 07
Charpy absorbed energy against temperature
Worked example · free
Peak stress and fracture stress on a brass rod curve
- 1Peak: 17,600 N divided by 50.27 mm² gives 350 MPa.
- 1Fracture: 15,080 N divided by 50.27 mm² gives 300 MPa.
- 1Drop: (350 minus 300) divided by 350 is 0.143, a fall of about 14%.
- 1The force fell because the rod thinned locally into a neck, so less force was needed to keep stretching it before it broke.
- 1Tensile strength is the maximum engineering stress, 350 MPa, not the 300 MPa at fracture.
Key terms
- Elongation After Fracture
- Permanent stretch of a broken tensile specimen, found from the gauge marks once the pieces are fitted together and expressed as a percentage of the original gauge length.
- Crosshead Displacement
- Distance the moving grip has travelled during a test, which includes grip seating and machine stretch as well as specimen extension.
- Charpy Impact Test
- Pendulum test that breaks a notched bar in one blow and reports the energy absorbed, as an indication of impact toughness.
- Proof Stress
- Stress at which a line parallel to the elastic slope, shifted by 0.002 strain, meets the measured curve.
- Necking
- Local thinning of a ductile specimen after the peak load, which lowers the force it can carry before fracture.
Tensile Testing and Charpy Impact FAQ
Why does my stress curve fall before the specimen breaks?
After the maximum load a ductile specimen starts to thin in one region. Because engineering stress divides by the original area, the reduced force shows as a falling curve even though the metal is still intact, so the peak, not the end point, is the tensile strength.
Can I use crosshead travel to work out elongation?
No. The grips' movement includes seating, machine compliance and stretch outside the marks, so the lab measures elongation after fracture from the distance between the original gauge marks with the halves reunited, and reports N/A when that cannot be measured.
What units should engineering stress be in?
Convert force to newtons and keep area in square millimetres, because one newton per square millimetre equals one megapascal. Leaving force in kilonewtons makes the result a thousand times too small, a common slip in this analysis.
What does Charpy absorbed energy actually measure?
It is the energy the notched specimen takes from the swinging pendulum, read in joules with machine corrections. It indicates impact toughness for that notch, size and temperature, and it should not be treated as fracture toughness or as a safe load for a real component.
How should I describe the change in Charpy results with temperature?
Keep each result as its own marker against temperature and resist drawing a smooth curve through a few points. The lab handout warns against assigning an exact transition temperature unless there is enough data and an agreed criterion for defining it.
Assessment move
Build one spreadsheet that takes width, thickness or diameter, gauge lengths and the exported force column, and outputs stress, tensile strength and elongation, then test it on an invented specimen whose answer you already know. Practise reading a stress curve aloud: where the peak is, where necking begins and where fracture occurs.
For impact work, practise turning pendulum heights into absorbed energy and applying a free-swing correction, using invented heights. Finally, write down which results came from crosshead data and which would need a measured strain.
Working through Tensile Testing and Charpy Impact in 40366? Sia is AskSia’s AI Engineering tutor — ask any 40366 Tensile Testing and Charpy Impact question and get a clear, step-by-step explanation grounded in how 40366 is taught and assessed. Read this chapter free, then take your hardest questions to Sia.